Picture two filter cores on a workshop bench. Same make of ceramic, same colour, same dimensions, the same neat checkerboard of plugged cells on the end face. One came from a good batch and the other from a poor one, or one is new and the other has been cleaned several times, or one is uncoated and the other carries a catalyst. Ask a visitor which one filters better and they will point at one with total confidence. They will be guessing. This guide to RECD filter porosity explains why the figure cannot be judged by looking at the core.
The property that decides the answer is porosity, and it lives inside the walls at a scale far below what the eye can resolve. This article explains why a retrofit emission control device (RECD) buyer cannot judge it by looking, what the word “porosity” actually bundles together, how six common look-alike situations fool inspection and what evidence works instead. We offer four numbers behind one word, six look-alike pairs, a certificate decoder and a short list of checks you can do without a laboratory. The advice is general. The filter maker’s data for your core takes priority, and any laboratory test should follow a stated method.
Why the eye cannot do this job
A ceramic wall-flow filter works because its walls are full of tiny interconnected voids. Exhaust gas has to squeeze through those voids to get from an inlet channel to an outlet channel, and soot particles are caught on the way. The voids that matter are measured in micrometres. A patent describing a filter for compression-ignition engines gives example mean pore sizes in the range of 8 to 45 micrometres, with 10 to 20 micrometres as one preferred band (US 9261004). The unaided eye can resolve detail of roughly a tenth of a millimetre, which is about a hundred micrometres. A pore of 15 micrometres is several times smaller than the smallest thing you can see, and the structure that matters is inside the wall, not on its surface.
What you see on a core is the end face, the skin, the plugs, the colour and any visible damage. These tell you about handling and gross defects. They say nothing about how many voids the walls hold, how large they are, how well they connect or whether ash has filled them. That is why inspection by appearance is a poor substitute for data.
Four numbers behind one word
“Porosity” in everyday speech means “how porous”, but in engineering the word is only one of several measurements that describe the wall. Four numbers matter.
| Number | What it is | What it mainly controls | How it is usually measured | What appearance shows |
|---|---|---|---|---|
| Total porosity | The percentage of the wall’s volume that is void | Overall resistance to flow; strength and stiffness | Mercury intrusion, or density and imaging methods | Nothing |
| Mean (median) pore size | The typical diameter of the voids, in micrometres | Which particles are caught and how deeply soot enters | Mercury intrusion porosimetry, sometimes with image analysis | Nothing |
| Pore size distribution | How wide the spread of sizes is, often written as d10, d50 and d90 | Pressure drop at a given soot load; whether a few big pores let particles through | Mercury intrusion porosimetry | Nothing |
| Pore connectivity and permeability | How well voids link up into flow paths | Pressure drop; how easily gas passes | Flow measurements through a wall sample or whole core | Nothing |
A US patent on cordierite structures lists these factors together when explaining pressure drop: the increase at a given soot load is influenced by the porosity, the median pore diameter, the width of the pore size distribution, the pore connectivity and how far the soot penetrates the walls (US 7141089). The same document explains that pore size distribution measured by mercury intrusion is expressed as d10, d50 and d90, the diameters at which 10, 50 and 90 percent of the mercury has intruded.
Because the four numbers are partly independent, a single figure such as “55 percent porosity” cannot describe a wall. Two walls with the same total porosity can behave differently.
How the numbers pull in different directions
Another patent makes the point plainly: porosity relates to back-pressure, with lower porosity generally giving higher back-pressure, yet a substrate of high porosity can be a poor filter if its mean pore size is also high (US 8608820). A third patent reports that particulate filters made with a mean pore size above about 30 micrometres show reduced filtration efficiency (US 12370479). So the buyer’s wish list of “high porosity for low back-pressure” and “small pores for high capture” has to be balanced by the maker, and the balance is only visible in the numbers.
Strength sets a third limit. A materials-science page on filter ceramics notes that porosity substantially reduces stiffness and that diesel filters need high porosity anyway (DoITPoMS). A study on cordierite found that mechanical properties such as strength and fracture toughness decrease as porosity rises, while thermal expansion is insensitive to porosity (US Department of Energy, OSTI). So a more porous wall is not automatically better. It is easier to push gas through but weaker, and the maker has to find a compromise between flow, capture and robustness.
Six look-alike pairs that fool inspection
Each of the pairs below looks the same from outside. Each has a different story inside.
Pair 1: same porosity, different pore size
Two cores can have the same total porosity, say 50 percent, with one built from fine pores and the other from coarse ones. A laboratory study of diesel filtration explains that the average diesel particle is much smaller than the mean pore size of a wall-flow filter, so particles are caught by diffusion to the pore walls and deposited there, and as the pores fill and bridge, filtration shifts to the soot cake (Cambustion). Pore size therefore shapes the early capture of a clean filter, while total porosity does not tell you that.
Pair 2: same pore size, different connectivity
If one wall’s voids are well connected and the other’s are mostly dead ends, gas will flow easily through the first and with difficulty through the second. The porosity and mean pore size can be identical. The difference appears as pressure drop at a given flow, which is why a flow test on the whole core reveals what the pore table cannot.
Pair 3: the new core and the ash-loaded core
Ash particles settle in the channel and enter the pores. A US laboratory study that imaged the pore structure of cordierite filters found that coating and ash loading blocked pores that had been open, raised pressure drop and affected the middle and rear of the filter in particular (US Department of Energy, OSTI). A core that has seen ash can look similar to a new one at the face yet have a different pore structure inside. For the buyer of a refurbished or used core, this is the central risk. See refurbished RECD filter core reuse and how to tell if an RECD filter is ash-loaded.
Pair 4: coated and uncoated
A catalytic washcoat sits on the walls and partly inside the pores. The patent on compression-ignition filters links washcoat loading to the filter’s mean pore size and backpressure, stating that particular combinations of pore size and loading give a desirable mix of filtration, catalytic activity and acceptable back-pressure (US 9261004). A coated core can look very like a bare one, and the pore structure differs. See catalysed versus uncatalysed RECD filters.
Pair 5: same colour, different batch or material
Cordierite and silicon carbide can both appear as grey or off-white blocks with similar faces, and a lot-to-lot change inside one material can alter pore structure without any visible sign. This is why a traceable lot number and a datasheet for that lot are better evidence than a family resemblance. See silicon carbide versus cordierite RECD filter substrate.
Pair 6: cleaned and not cleaned
A core that has been through a cleaning process may look clean at the face while retaining residue in the pores. After cleaning, the useful test is not appearance but pressure at a reference flow compared with the clean baseline. See RECD pressure high after a cleaning service and verifying that an RECD cleaning report shows the service was effective.
Even the lab numbers have limits
It would be tidy to say that a mercury-porosimetry certificate settles everything. It does not. An SAE paper on pore structure notes that filtration efficiency is generally lower for materials with higher porosity and pore size, but that this is not always supported by experimental correlations between efficiency and mercury porosimetry data, and proposes combining porosimetry with image analysis to describe the structure better (SAE 2007-01-1918). In other words, even the standard lab numbers are a simplification.
The sensible conclusion is not to distrust data but to read it as a set. A datasheet that gives porosity, mean pore size and distribution and performance measured on the actual core (clean pressure drop at a stated flow, filtration efficiency with its test method) tells you much more than any one pore number.
Certificate decoder: what each statement should come with
A supplier’s datasheet or lot certificate should answer the questions in the middle column. If it does not, ask the question in the right column.
| Statement on the paper | What it should include | Question to ask |
|---|---|---|
| “Porosity 55 %” | The measurement method, the sample location and the tolerance | How was it measured and on which sample from the lot? |
| “Mean pore size 15 µm” | Method and the pore size distribution (d10, d50, d90) | Can you provide the full distribution? |
| “High efficiency” | Test method, particle size or count basis, soot condition and temperature | Is this clean or soot-loaded efficiency, and by what test? See RECD particle number versus particle mass |
| “Low pressure drop” | Flow, temperature, clean or loaded state | At what flow and soot load, and is it a measured core or a design value? |
| “Made from premium cordierite” | Material grade and lot traceability | Can you link this core’s serial number to a lot test record? |
| “Same as OEM” | Matching cell density, wall, porosity and size | Where is the comparison datasheet? |
Checks you can do without a laboratory
You cannot see porosity, but you can collect evidence that is influenced by it. None of the checks below replaces laboratory data. Together they make a decent screen.
- Ask for the lot and serial number and a test record. Traceability is the base of everything else. A core without one is an unknown.
- Weigh the core. Mass depends on geometry, material and porosity. Compare it with the supplier’s stated mass and with a sister core of the same model. A deviation does not say which property differs, but it flags a core that needs a question. Ask the supplier for the stated tolerance.
- Measure the dimensions with a tape or calliper against the drawing. Out-of-tolerance dimensions can indicate a poor batch or damage.
- Ask for a flow-bench result. A pressure drop at a stated flow, measured on the actual core and compared with the clean reference for the model, is the most direct functional check of the whole pore system.
- Witness a test where the order justifies it. See factory acceptance versus site acceptance tests for RECD projects and questions to ask during an RECD factory visit.
- Photograph and document at delivery. Condition, plugs, skin and marks. See the RECD delivery inspection checklist.
- Record a baseline. After installation, note the pressure at a reference load. Later changes in pressure at the same load tell you about the wall in service. See comparing RECD pressure readings at different generator loads.
- Keep a retained sample if the supplier will provide one. Some suppliers can retain a coupon from the lot for later analysis if a dispute arises.
What porosity does once the filter is running
Porosity is not fixed. In service the pore structure changes in three ways, and the changes explain why a filter that was perfectly sized on day one can drift.
- Soot loading. Early in loading, soot penetrates the pores and raises pressure drop sharply, and later the cake forms on the surface. A filter’s behaviour in that first phase depends strongly on pore structure.
- Ash build-up. Ash settles on the wall and partly in the pores, and it stays after regeneration. The US laboratory study cited above documented the pore changes. See soot versus ash in RECD regeneration.
- Thermal and chemical ageing. Repeated high-temperature cycles and chemical exposure can change the wall and any coating. See catalyst ageing and RECD regeneration behaviour.
For the buyer this means that appearance at the end of a core’s life tells even less than at the start. Condition-based assessment, using pressure at a reference load and the supplier’s laboratory findings at cleaning, tells the real story. See RECD cleaning intervals by calendar, hours or condition.
A worked illustration: two identical-looking cores
The following is an illustrative scenario, not a real customer or product. A hotel group needs a replacement core for a 400 kVA set and receives two offers. A dealer offers a “new-old-stock” core at a lower price, and the original supplier offers a new one. The hotel’s engineer inspects both on a bench: same dimensions, same colour, clean faces, neat plugs. The dealer’s paperwork says “same specification”. The engineer decides to apply the checks.
Traceability. The supplier’s core has a serial number linked to a lot test record that lists total porosity, mean pore size with the distribution, the measurement method and a flow-bench result. The dealer’s core has a label with a part number only.
Weight. The supplier’s core matches its stated mass within the stated tolerance. The dealer’s core is about a tenth lighter than the supplier’s data for the model. The dealer says old stock varies. The engineer notes that a lighter core could mean a different wall structure, a different model or damage, and that the difference cannot be resolved by looking.
Flow. The hotel asks both sellers for a flow-bench result at the same stated flow. The supplier provides one, and it falls close to its reference. The dealer offers to run a test only if the hotel buys.
Decision. The hotel decides it cannot verify the dealer’s core and declines it, keeping a note of the reasoning. It buys the traceable core and records the pressure at its reference load after installation as the baseline. Over the first months, pressure at the reference load stays close to that figure, and at the first cleaning the supplier’s report compares the cleaned core’s pressure with the baseline.
Lesson. The two cores looked the same, and the difference between them was paper and measurements. The hotel did not need to know pore sizes. It needed a supplier who could show them.
Questions to put to a supplier
- What are the total porosity, mean pore size and pore size distribution, and by what method were they measured?
- Are the figures from this lot, and can you give the lot and serial number?
- What are the clean and loaded pressure drops of this core at my engine’s flow and temperature?
- What is the filtration efficiency, by mass and by particle number, and on what test and soot condition?
- How does the washcoat, if any, change the pore structure and back-pressure?
- What is the core’s mass, and the tolerance?
- What happens to the pore structure in service from ash and ageing, and how do you check it at cleaning?
- Can you retain a sample or provide a witnessed flow test?
Mistakes to avoid
- Judging a core by its face. Pores are invisible.
- Reading “porosity” as a single quality score. Pore size, distribution and connectivity matter too.
- Believing high porosity means low back-pressure always. Pore size and connectivity can undo it.
- Accepting a datasheet without a method or lot.
- Reusing an unverified used core that looks clean.
- Ignoring a baseline. Without one, later drift cannot be interpreted.
- Assuming a laboratory number settles performance. Combine it with flow and efficiency data.
Questions people ask
What is a good porosity for an RECD filter?
There is no single figure. Patent examples describe total porosities spanning wide ranges, often between about 40 and 75 percent depending on the material and design, but the right value depends on pore size, strength and the maker’s balance of back-pressure and capture. Ask for the data and the justification.
Can I tell porosity by weight?
Weight carries some information, but it also depends on geometry and material. It can flag a core that needs questions. It cannot isolate porosity.
Does a higher porosity filter capture less soot?
Not necessarily. Capture depends on pore size, distribution and the soot layer as much as on total porosity. A very coarse pore size can reduce efficiency, whatever the total.
Can cleaning restore porosity?
Cleaning can remove soot and some ash, but residue may remain in the pores. Compare pressure at a reference load after cleaning with the clean baseline, and read the cleaning report.
The takeaway
Porosity is not a look. It is four numbers hidden inside the wall, and a core’s behaviour depends on how they combine, how they change in service and whether the maker’s data was measured on a core like yours. Buy on traceability, datasheets with methods, flow evidence and a baseline, and treat any claim based on appearance as an opinion. Want a second pair of eyes on an offer or a report? Contact Aceget, read the FAQ or look through our retrofit emission control devices.
Related Reading
- RECD Filter Cell Density: What Does CPSI Mean for Buyers?
- Refurbished RECD Filter Core Reuse
- How to Tell if an RECD Filter Is Ash-Loaded
- RECD Delivery Inspection Checklist
- Silicon Carbide vs Cordierite RECD Filter Substrate
Sources
- US patent 9261004: filter for particulate matter from a compression ignition engine
- US patent 7141089: magnesium aluminium silicate structures for DPF applications
- US patent 8608820: filter for particulate matter, porosity and pore size
- US patent 12370479: honeycomb body with porous material
- SAE 2007-01-1918: pore structure and filtration efficiency characterisation
- Cambustion: DPF testing, pressure drop and filtration efficiency
- US Department of Energy, OSTI: pore structure of cordierite filters with ash and coating
- US Department of Energy, OSTI: porosity and microcracking in cordierite
- DoITPoMS: diesel particulate filter materials