A cracked filter core is one of the quietest failures an RECD can have. The housing looks the same, the controller still shows a pressure and the set carries its load. Inside the canister, a ceramic block that was meant to force every gram of exhaust through its walls may have split, and some of the gas is now taking a shortcut. This guide to a cracked RECD filter substrate explains what the cracks mean and what evidence settles the cause.
The difficulty is that cracks do not announce themselves. A peer-reviewed study of cordierite filters from a commercial fleet describes a crack that ran through the whole cross-section, close to the outlet face, and that could not be seen until the filter was cut in half (Springer, Emission Control Science and Technology). Nothing on the outside of that filter suggested what was inside. For a plant owner who has to decide whether to keep running, send the core for repair or buy a replacement, the practical question is not “is there a crack?” but “what evidence would convince a reasonable person that there is, or is not, one?”
This article is built around that question. We sort cracks into five patterns, list five stress sources that make ceramic crack, give a six-rung evidence ladder from the cheapest check to the most conclusive and show what a cracked core does to the readings you already collect. A comparison with look-alike failures and a worked illustration complete the picture. The advice is general. The filter maker’s inspection method and the engine maker’s guidance take priority, and opening a filter housing or examining a core belongs to the supplier or a qualified technician.
What a crack changes inside an RECD
To see why cracks matter, recall what the core is for. In a wall-flow filter, alternate channels are blocked at opposite ends, so exhaust cannot pass straight through. It has to cross the porous channel wall, and the wall holds back the soot. That forced crossing is the whole filtration mechanism.
A crack in the ceramic breaks that rule. Gas finds the gap, takes the easier route and carries soot with it. Three things follow.
- Soot escapes. The crack acts as a leak around the filtering walls. A numerical study of damaged filters published by SAE examines how a damaged core changes pressure loss and lets soot leak through (SAE 2009-01-1267). The details depend on the size and position of the damage, but the direction is clear: less soot is held back.
- The pressure picture changes. A bypass path can make the pressure drop lower than the soot load would predict. That is the opposite of what most operators watch for, because most alarms are set for high pressure.
- Further damage becomes more likely. A cracked core can move, rub on its support and break at the edges, so a hairline can become a gap in a few hundred hours.
That is why crack detection is not simply a matter of waiting for a high-pressure alarm. First, we need a vocabulary for cracks.
Five crack patterns and what they usually mean
Not every crack is the same kind of event. The pattern gives a clue about the stress that caused it.
| Pattern | What it looks like | Usual direction | Typical story |
|---|---|---|---|
| A. Transverse or ring-off crack | A crack running across the core, perpendicular to the flow, often splitting it into two pieces | Across the axis | A thermal gradient along or across the core that exceeded the ceramic’s strength |
| B. Radial or star crack | Cracks fanning outward from the centre or from a point on the end face | Across the face | Hot centre and cool edge during regeneration, or a local hot spot |
| C. Longitudinal crack | A crack running along the length of the core, between channels | Along the axis | Mechanical load from canning or support, or severe radial temperature difference |
| D. Face or edge crack or chip | Damage at an end face or outer skin, sometimes a broken corner | Local | Handling, impact, over-tight clamping, plug loss, or erosion at the edge |
| E. Microcracks | A network of very fine cracks inside the ceramic that cannot be seen by eye | Microscopic | Often a deliberate feature of the material, not a fault |
Pattern A: the ring-off crack
An SAE paper on catalysed silicon carbide filters defines ring-off cracking as a crack caused mainly by thermal gradients and the stresses they produce inside the core, where the stress exceeds the strength of the material. It adds that these cracks usually run perpendicular to the flow axis and typically separate the core into two halves (SAE 2008-01-0765). The same paper treats filtration efficiency as a possible indicator that such a crack has occurred, which supports the idea that capture performance, not just pressure, is evidence.
Two practical points follow. “Ring-off” is a pattern name, not a material name, so any ceramic core can show it if the gradient is steep enough. And because the two halves may stay roughly in place inside the canister, the filter can behave normally at first, revealing itself only when a vibration, load change or cleaning job moves the halves.
Pattern B: radial cracks
A hot centre with a cool rim is a classic recipe. A European patent on cordierite honeycombs describes a core that can sit at 800 to 1,000 degrees Celsius near the centre while the periphery near the skin is at 400 to 500 degrees, a difference that builds stress across the radius (EP 1957180). Radial cracks are one way that stress is relieved. They tend to appear when regeneration is concentrated in the middle of the core, which happens when soot is not evenly loaded or when flow is skewed toward the centre. Our article on RECD regeneration temperature explains how heat is generated and where it goes.
Pattern C: longitudinal cracks
A crack that runs along the length points the investigation toward forces and tolerances. The core is held by a wrapped mat inside a steel shell, and a mat that squeezes too hard or unevenly, or a shell distorted by heat or a knock, can load the block. See our companion article on canning and the substrate support mat.
Pattern D: face and edge damage
Ends and edges take the knocks: a dropped core, a slipping tool or a tight gasket can chip an edge. Face damage can also be the first sign that an end plug has loosened or fallen out; see what end plugs do in wall-flow filtration.
Pattern E: microcracks are not always a defect
Some cordierite is deliberately microcracked. A US patent on low-microcracked honeycombs explains that high thermal shock resistance has historically been achieved by keeping the coefficient of thermal expansion low, which is attained partly through microcracking and crystal orientation in the ceramic (US 8501296). Those microcracks are part of the material design and are not what this article means by a cracked substrate. If a report mentions “microcracking” in a new core, ask whether it describes the normal microstructure.
Five stress sources: why ceramic cracks
Ceramic is hard and heat-resistant but not tolerant of being stretched. It cracks when the stress inside it exceeds what it can bear. Five sources of stress account for most cracks. A failure investigation should ask which of them was present.
1. Thermal gradient during regeneration
When soot burns, it releases heat inside the core. If the burn is concentrated, the hot zone expands while the cooler zone around it does not, and the mismatch stresses the ceramic. Melting and thermal-shock failure have long been recognised as significant regeneration issues in ceramic honeycomb filters (SAE 870010). The risk grows with the soot burnt in one event and the unevenness of the soot layer.
A related event is the sudden drop in engine load during a burn, sometimes called a drop to idle. SAE research reports that it can create a transient temperature peak much higher than steady-state burning, enough to cause local melting or cracking (SAE 2014-01-1561). On a DG set, the analogue is a load trip or breaker opening during a regeneration. See what happens when a generator stops during RECD regeneration.
2. Thermal shock from a rapid temperature change
Rapid cooling or heating is a separate stress. Water on a hot core, a cold start on a heavily loaded filter or a coolant leak into the exhaust each subject the ceramic to a fast temperature change. We give this topic its own article, can thermal shock damage an RECD filter?
3. Mechanical load and vibration
A filter core is held in place by friction and compression. Over-compression during canning, a loose mat that lets the core move, resonance from the exhaust line, a hard hit during transport or a poorly supported housing can all load the ceramic. See packaging and transporting an RECD without damage and how to prevent generator vibration issues.
4. Ash and alkali chemistry
The same fleet study that described the hidden crack also linked failures to the chemistry of the deposit. It reports that alkali compounds were reported to lower the melting point of cordierite and silicon carbide to roughly 700 to 900 degrees Celsius, a range that overlaps with temperatures seen in controlled regeneration. It also notes that crack failures showed the same crystalline phase changes as melt failures and suggests that differing thermal expansion among crystalline phases could be involved (Springer). The authors stress that evidence linking operational failures to ash chemistry is limited, so treat this as a line of enquiry, not a rule. For the chemistry side, see catalyst poisoning in an RECD and soot versus ash in RECD regeneration.
5. A flaw that was already there
Manufacturing variation, a crack that formed during canning or a small chip from handling can start as a defect and grow in service. This is why a delivery inspection and a post-installation baseline are worth the effort. See the RECD delivery inspection checklist.
The six-rung evidence ladder
Inspection should start with the cheapest evidence and climb only as far as the decision requires. Each rung is stronger than the one below it, and each has limits. Record what you did at every rung, even if the result is “nothing found”.
Rung 0: the records
What to do. Pull the controller log for the weeks around the suspect event: pressure at a reference load, inlet and outlet temperatures, regeneration events, alarms and load changes. Add the service history, the date of the last cleaning and any incidents (a trip, a water leak, a transport move, a repair). See what to record in an RECD event log and what an RECD regeneration history report should contain.
What it can show. A dated step change, such as a pressure that fell suddenly after a regeneration, and a candidate stress source. It cannot show whether the core is cracked, because a step can also come from a sensor fault, a blocked tapping or a leaking joint. See separating a sensor fault from an RECD performance problem.
Rung 1: outside observation
What to do. Walk the exhaust path with the set stopped and cool. Look at the outlet pipe and the stack for fresh soot streaks, which indicate that soot is escaping the filter. Check the outlet side of the housing for staining at joints. Listen when the housing is tapped gently with a soft mallet by the supplier’s technician: a loose, rattling core sounds different from a firmly held one. Check for new smoke at the stack at steady load.
What it can show. Signs of soot leakage and of a loose core. Soot at the stack can also come from a gasket leak or engine condition, so treat it as a pointer, not a proof.
Rung 2: end-face inspection
What to do. With the supplier, remove an access cover or open the housing in a safe, clean setting and examine both end faces with a bright torch and a camera. Take photographs with a scale reference. Look for broken corners, displaced plugs, cracks on the face, patterns of unusual soot on the outlet face and gaps between the core and its support.
What it can show. Face cracks, plug loss, edge damage and bypass marks. A clean outlet face is expected in a healthy core, and a sooty one is a red flag. Internal cracks, which can lie some way from either face, stay hidden.
Rung 3: endoscope or borescope
What to do. Use a small camera to look down individual channels from the outlet face, with the supplier’s approval, and sample several areas. Look for soot where there should be none, cracks that cut across channels and burned or glazed areas.
What it can show. Channel-level evidence of cracks and melt near the face. A borescope views only a thin slice of a large volume, though: a clear view of ten channels says nothing about the other ten thousand.
Rung 4: flow, leak or back-pressure test
What to do. Ask the supplier to test the core on a flow bench or in a leak test setup. A flow test compares the pressure drop of the suspect core with that of a clean reference of the same type, at the same flow. A smoke or tracer test can reveal a path that bypasses the walls. Some suppliers also run an efficiency check, taking particle readings upstream and downstream.
What it can show. A core that passes air more freely than its twin, or leaks tracer where it should not, is behaving as if cracked, and efficiency testing goes straight to the function that matters. It cannot locate a crack, and a hairline may not change flow noticeably.
Rung 5: teardown and cross-section
What to do. Cut the core in a controlled way, photograph the cut faces, and take samples for chemical analysis. This is destructive, so it is done when the decision justifies it: a warranty dispute, a repeat failure or a need to know the root cause.
What it can show. The crack’s position, width and path, whether faces are glazed or melted and the chemistry around the damage. A cross-section tells you what happened; the records tell you why.
Reading the ladder
| Rung | Cost and effort | Strength of evidence | Stop here if |
|---|---|---|---|
| 0. Records | Low | Pointer only | The records clearly show a sensor fault and the core passes rung 2 |
| 1. Outside | Low | Pointer only | No soot at the outlet, no rattle, readings stable |
| 2. End faces | Medium | Direct for face damage | Faces are sound and efficiency is acceptable |
| 3. Endoscope | Medium | Direct but narrow | Several areas are clean and flow is normal |
| 4. Flow or efficiency test | Medium to high | Strong for function | Results match a healthy reference |
| 5. Teardown | High | Conclusive | The cause must be established for a claim or design change |
The rule of thumb is to climb until the decision is safe. If a cleaned core passes a flow test and an efficiency check and shows no face damage, the evidence is strong enough to carry on. If the core leaks tracer, there is little to be gained from spending more on a borescope.
What a cracked core does to your usual readings
A suspected crack is easier to judge when you know the patterns it can leave in routine data.
| Reading | What a crack can do | Caution |
|---|---|---|
| Pressure drop at a reference load | May fall below the level expected for the soot load, or drop suddenly after an event | A drop can also come from a blocked tapping or a leak; a rise is still possible if the crack is small |
| Loading rate | May appear to slow because soot bypasses the walls | Slower loading can mean the filter is less effective, not that the engine is cleaner |
| Outlet smoke or opacity | May rise, particularly on load steps | Needs a baseline. See smoke opacity versus particulate mass |
| Measured particulate downstream | May rise if a laboratory or analyser is used | Sampling location and dilution can distort the result. See exhaust sampling location |
Particle-number measurements can reveal bypass even when mass readings look modest. See particle number versus particle mass.
Cracks compared with three look-alikes
A good investigator separates a crack from three other failures that leave similar clues.
| Failure | Distinguishing evidence | Why it is confused with a crack |
|---|---|---|
| Melt | Glassy, fused, slumped or glazed ceramic; voids where channels have merged; often near a hot zone | Both create a bypass and a falling pressure |
| Plug loss | Missing or loose plugs on the end face; local bypass of single channels | Also lets soot through |
| Erosion or pinholes | Small holes through channel walls; localised wear | Also creates leakage paths |
| Seal or mat leak | Soot between the core and the can; staining at the shell | Soot appears at the outlet without a crack in the ceramic |
The fleet study mentioned earlier classified failures into pinhole, melt, crack and fouling types, which shows how many routes lead to the same symptom (Springer). Our companion article on what a failure investigation should cover for melted cells deals with the melt branch in detail.
When you suspect a crack: do and do not
Do stop and preserve the evidence: photograph the housing and outlet, save the log, ask the supplier how long and at what load the set may run before inspection and agree a written inspection scope. Keep the removed core until the cause is agreed.
Do not force a regeneration to see whether pressure recovers, because heat on a cracked core can enlarge the damage. Do not wash or blow out the core: water, compressed air and impact can widen a crack and destroy evidence (see can you wash an RECD filter? and compressed-air cleaning of RECD filters). Do not patch a crack with cement unless the supplier has a documented method for your core type, do not raise alarm limits to hide a falling pressure and do not reuse the core on a verbal assurance. See reusing a refurbished RECD filter core.
A worked illustration: the pressure that fell
The following is an illustrative scenario, not a real customer. A packaging plant runs a 500 kVA set with an RECD. At a reference load of about 75 percent, the filter’s pressure drop has been climbing slowly since the last cleaning, as expected. One Monday morning the shift log shows a trip during a mains restoration test the previous Friday, followed by a pressure reading that is now about 40 percent lower than the Thursday figure at the same load. The pressure alarm is quiet, and the operator is pleased that the filter “seems cleaner”.
Rung 0. The controller log shows that the trip happened while an active regeneration was in progress. The inlet temperature rose sharply for several minutes before the set stopped, and the pressure fell in steps rather than gradually afterwards. The team lists the candidate stress source: a thermal gradient with a load drop during a burn.
Rung 1. A walk-round shows fresh dark streaks on the outlet pipe flange and a faint grey haze at the stack on load steps. The supplier’s technician taps the housing and hears a dull knock that he does not hear on the sister set.
Rung 2. At the supplier’s workshop the core is examined. The inlet face carries a moderate soot layer. The outlet face shows a band of soot staining across about a third of its width and a hairline visible near the edge.
Rung 3. A borescope view down several channels at the stained area shows soot lining channels that should be clean, and a crack crossing the channel walls.
Rungs 4 and 5. A flow test shows a pressure drop about a third lower than a healthy core of the same type at the same flow, and a tracer test confirms a path around the walls. Because the plant wants a root cause for a warranty discussion, the core is sectioned: a transverse crack runs through the full cross-section, with no melting nearby. The report records a ring-off pattern after a regeneration interrupted by a load trip.
Decision. The core is replaced, the housing support is inspected and the controller’s regeneration logic is reviewed with the supplier so that regenerations are not started when a load test or transfer is scheduled. The plant adds a rule to the maintenance calendar: no active regeneration within a set window before planned transfer tests. See RECD regeneration inhibit signals.
What a good supplier report on a cracked core contains
Ask for a written report that identifies the core and its service history, shows photographs of both end faces and the skin with a scale, names the crack pattern, position and extent, weighs the evidence for each stress source against the records, gives any flow or efficiency test result with its reference and states whether the cause is a defect, an operating issue or undetermined, with corrective actions. Compare it with our guidance on auditing an RECD service report for missing information and what to record in an RECD warranty claim.
Reducing the chance of a crack
- Keep soot loading in check, since burning a heavy load releases more heat. See how often an RECD regenerates.
- Schedule burns away from load transitions such as transfer tests.
- Protect the hot core from water. See RECD protection from rainwater and condensation.
- Check the mounting and handle with care during transport, storage and servicing.
- Take a baseline pressure reading at a reference load after installation or cleaning. See comparing RECD pressure readings at different generator loads.
Mistakes to avoid
- Treating a falling pressure as good news without asking why.
- Judging a core from the outside.
- Calling microcracks a defect when they are part of the material’s design.
- Stopping at the borescope, which views only a small part of the core.
- Washing or blowing out a suspect core before it is examined.
- Replacing the core and ignoring the cause, or discarding the failed core, which is the best evidence available.
Questions people ask
Can a cracked RECD filter still work?
It may keep trapping part of the soot, but its efficiency is reduced because gas can bypass the walls. How much is lost depends on the crack’s size and position, and this has to be measured, not assumed.
Will the pressure alarm warn me?
Not necessarily. Most alarms are set for high pressure. A bypass crack can lower pressure, so a sudden unexplained drop deserves attention too.
Can a cracked core be repaired?
Some suppliers have documented repair methods for particular cores. Ask for the method, the tests that prove it and any warranty on the repair. A repair without evidence is a risk.
The takeaway
A crack in an RECD core does not shout. It leaves quiet clues: a pressure that fell, soot where there was none and a knock in the housing. Sort the crack by pattern, ask which of five stress sources was present, climb the evidence ladder only as far as the decision needs and keep the removed core and the records. Questions about your own set? Start with our retrofit emission control devices, check the FAQ or talk to the Aceget team.
Related Reading
- Melted RECD Filter Cells: What a Failure Investigation Should Cover
- Can Thermal Shock Damage an RECD Filter?
- Repeated Failed Regeneration and RECD Filter Damage
- Silicon Carbide vs Cordierite RECD Filter Substrate
- RECD Filter Core vs Complete Assembly Replacement
Sources
- Springer, Emission Control Science and Technology: failure modes in cordierite DPF substrates
- SAE 2008-01-0765: ring-off cracks in a catalysed silicon carbide DPF
- SAE 2009-01-1267: pressure loss and soot leakage through a damaged DPF
- SAE 870010: cell structure and regeneration failure of ceramic honeycomb filters
- SAE 2014-01-1561: maximum temperature rise following a drop to idle
- US patent 8501296: stabilised low-microcracked ceramic honeycombs
- European patent EP 1957180: cordierite honeycomb thermal gradients